Inkjet coding of 7075-T651 on aluminum plates

Why Do Black Spots Appear After CNC Machining 7075 Aluminum Plate?

What are the black spots on CNC machined 7075 aluminum plates?

After CNC machining 7075 aluminum plates (12.2 × 1560 × 6400 mm), some customers report dark black patch-like marks​ on the surface.

Key characteristics:

  • Appearance: dark black, irregular patches
  • Depth: only 0.02–0.03 mm​
  • Microstructure: shallow, no cutting deformation
  • Removal: disappears completely after light surface grinding

✅ Conclusion:​ These are surface corrosion marks, not CNC machining defects.

Are these black spots caused by CNC machining?

No.

CNC machining only exposes the existing surface condition of the aluminum plate.

Typical CNC-related defects include:

  • Tool marks
  • Scratches
  • Chatter marks
  • Heat discoloration

Corrosion black spots are not generated during machining.

Why is 7075 aluminum prone to surface black spots?

  1. Material nature (root cause)
  • 7075 is a high-copper, high-strength aluminum alloy​
  • Excellent mechanical properties
  • Poor corrosion resistance compared to 5052, 5083, or 6061

When exposed to moisture, chlorides, or acidic environments, surface corrosion occurs easily.

  1. Common causes before machining
  • Incomplete cleaning after rolling → residual oil, chloride, acid
  • Poor passivation → uneven protective film
  • Bare-hand contact → sweat (chloride) left on the surface
  1. Storage & transportation factors
  • High warehouse humidity (>50% RH)
  • Temperature fluctuations → condensation
  • Long storage time → trapped moisture
  • Poor packaging → water vapor penetration

How to confirm it is corrosion, not machining damage?

You can verify using three simple checks:

Check Method Result
Visual inspection Black patches, no tool marks
Depth measurement ≤ 0.03 mm
Light grinding Defect fully removed

If all three match, the issue is pre-existing surface corrosion.

How to prevent black spots on 7075 aluminum plates?

✅ At the production stage

  • Use pure water final rinsing​ to remove chlorides
  • Apply standardized chemical passivation​ (72h salt spray qualified)
  • Control humidity ≤ 50% RH in cutting & inspection areas
  • Prohibit bare-hand contact with plates

✅ During inspection & delivery

  • Strong-light visual inspection for every plate
  • Sample grinding verification (0.02–0.03 mm)
  • Salt spray testing for critical batches

✅ Packaging & storage

  • Moisture-proof film + desiccant + sealed wrapping
  • Humidity indicator cards inside packaging
  • Clear labeling: “Keep Dry – Store Flat – Do Not Stack”
  • FIFO inventory control (short storage cycle)

✅ During CNC machining

  • Unpack within 48 hours​ of arrival
  • Pre-inspect plate surface under strong light
  • Use rust-inhibiting cutting fluid
  • Clean and dry parts immediately after machining

Real case example

A customer reported black spots after machining a batch of 7075 plates.

Inspection confirmed shallow surface corrosion, removable by grinding 0.03 mm.

Root cause:

  • Residual chloride from incomplete cleaning
  • Moisture trapped in packaging

Corrective actions:

  • Upgraded to pure-water final rinse
  • Standardized passivation process
  • Improved moisture-proof packaging

✅ No recurrence in subsequent batches.

FAQ – Quick Answers

Q: Are black spots a material defect?​

A: No. They are surface corrosion, not internal material failure.

Q: Can CNC machining cause black spots?​

A: No. CNC only removes material and reveals pre-existing surface issues.

Q: Can I still use plates with black spots?​

A: Yes, if the corrosion depth is within allowable tolerance. Light milling removes it.

Q: Which aluminum alloy resists corrosion better?​

A: 5052, 5083, and 6061 offer better corrosion resistance than 7075.

Need help with 7075 aluminum quality control?

We supply 7075 aluminum plates, bars, and forgings​ with:

  • Strict cleaning & passivation control
  • Full EN 10204 3.1 inspection certificates
  • Export-standard moisture-proof packaging

Contact us for:

  • Technical consultation
  • Corrosion risk assessment
  • Custom cutting & surface treatment
0 replies

Leave a Reply

Want to join the discussion?
Feel free to contribute!

Leave a Reply

Your email address will not be published. Required fields are marked *