Aluminum Flat Tube

Case Study: Root Cause Analysis & Process Optimization for Aluminum Alloy Flat Tube Leakage

Case Study: Root Cause Analysis & Process Optimization for Aluminum Alloy Flat Tube Leakage

Executive Summary

This case study addresses a batch leakage defect​ in C3Q6-H14 aluminum alloy flat tubes (wall thickness 0.22 mm) used in heat exchangers. Through comprehensive mechanical testing, multi-station metallographic inspection, and full-process traceability, the failure was confirmed unrelated to raw material mechanical properties, but caused by process parameter deviation, inadequate inline control, and poor inter-process coordination.

Aluminum Flat Tube

The leakage consistently occurred at mechanical marking positions, where excessive wall thinning (up to 51.4%) led to structural weakness, flux accumulation, and high-temperature erosion during brazing, ultimately resulting in tube perforation.

A closed-loop corrective action plan was implemented, covering emergency containment, standardized process control, upgraded inspection systems, and long-term preventive mechanisms—significantly improving yield and product reliability.


Core Findings

Item Key Data
Normal marking area Min. wall thickness 0.146 mm (34% thinning)
Pre-brazing marking area Min. wall thickness 0.107 mm (51.4% thinning)
Failure mechanism Over-thinning → strength loss → brazing overheating & penetration
Root cause Non-standard marking parameters + missing wall thickness control
Systemic gaps No inter-process linkage, no micro-defect prevention

Corrective & Preventive Actions

  1. Immediate Containment
    • 100% inline and finished-product inspection
    • Isolation and rework/scrap of non-conforming units
    • Full equipment calibration (pressure, stroke, speed)
  2. Process Standardization
    • DOE-optimized marking parameters for 0.22 mm tubes
    • Wall thinning strictly limited to ≤30%
    • Mold life management and scheduled replacement
  3. Inspection System Upgrade
    • Macro: Precision wall thickness measurement + SPC monitoring
    • Micro: Weekly metallographic sampling to detect Cu/Fe segregation and inclusions
  4. Inter-Process Coordination
    • Dynamic brazing parameter adjustment triggered by wall thinning fluctuations
    • Real-time cross-process alert and correction mechanism
  5. Raw Material Enhancement
    • Added incoming metallographic inspection to screen micro-defects before processing

Long-Term Value

  • Eliminates chronic leakage risk in thin-wall aluminum flat tubes
  • Establishes a dual-layer quality system: dimensional + metallographic control
  • Builds scalable, traceable, and continuously improving process standards
  • Enhances confidence for high-reliability applications (HVAC, automotive, energy systems)