  1. Material Overview

7A62 is a high‑strength, weldable Al–Zn–Mg aluminum alloy standardized under GB/T 3190‑2020. Developed in 2013, it is recognized as the highest‑strength weldable aluminum alloy and China’s third‑generation armor material. Based on 7A52, it features higher zinc and magnesium contents and an optimized Cr–Zr composite grain refinement system, representing China’s advanced independent R&D capability in high‑strength weldable aluminum alloys.

Core Advantages

  • Ultra‑high strength: Quasi‑static yield strength up to 608 MPa; tensile strength >25 % higher than 7A52
  • Excellent weldability: Best‑in‑class among high‑strength 7000‑series alloys
  • High stress corrosion resistance: Enhanced via T7X overaging
  • Superior ballistic performance: High strength + good toughness for armor applications
  • Mature production: Mass‑produced for defense and special vehicles

Standards Compliance

  • GB/T 3190‑2020: Wrought aluminum chemical composition
  • T/COS 019‑2025: Weldable armor forgings
  • T/COS 020‑2025: Armor forgings
  • GJB 9614‑2019: 7B52 laminated armor sheets

Edition Notes

This report aligns with national standards, industry specifications, and commercial data. It covers 0.2 mm thin sheets to 300 mm extra‑thick forgings with full temper data (T4, T6, T651, T7X, H112) for drawing, material selection, procurement, and quality inspection.

  1. Full‑Thickness Application Guide
Thickness Range Product Form Recommended Temper Typical Applications
0.2–2.0 mm Thin sheet / strip T6, T4 Light armor skins, bulletproof shells, trim panels
2.0–6.0 mm Rolled sheet T6, T651 Armor panels, turret shells, protective liners
6.0–25 mm Medium–thick plate T6, T651, T7X Main armor structures, missile containers, guards
25–100 mm Thick plate T6, T651, H112 Tank frames, turret bases, armor supports
100–150 mm Extra‑thick plate T6, T651, H112 Heavy load frames, vehicle reinforcements
150–300 mm Extra‑thick forging H112, T6 Large armor forgings, heavy protective parts

Key Applications

  • 7B52 laminated armor: High‑strength layer (7A62) + tough layer (7A52) + core layer (7A01)
  • Defense: Armored vehicles, tanks, turrets, ballistic protection
  • Special vehicles: High‑strength structural components
  • Welded assemblies: Primary welded armor structures

III. Heat Treatment Specifications

  1. Solution treatment: 460–475 °C, water quench
  2. T6 peak aging: 120 °C / 24 h; maximum strength
  3. T7X overaging: Two‑stage; improves stress corrosion resistance
  4. T4 natural aging: Room temp ≥96 h; good pre‑weld plasticity
  5. Stress relief: 5–3 % tension for plates >25 mm
  6. Deep cryogenic treatment: Enhances strength/elongation
  7. Online quenching: Improves impact performance

Temper Definitions

  • T4: Solution + natural aging; pre‑weld state
  • T6: Solution + peak aging; highest strength
  • T651: Solution + tension relief + aging; thick plates
  • T7X: Solution + overaging; corrosion resistance
  • H112: Hot‑worked; extra‑thick forgings
  1. Chemical Composition (Mass Fraction, %)
Element Si Fe Cu Mn Mg Cr Zn Ti Zr Be Others (Ind.) Others (Total) Al
Limit ≤0.12 ≤0.15 0.05–0.50 0.20–0.60 2.5–3.2 0.10–0.20 6.7–7.4 0.03–0.10 0.05–0.15 0.0001–0.003 ≤0.05 ≤0.15 Balance

Key Notes

  • Ultra‑high Zn (6.7–7.4 %): Main strengthening phase (MgZn₂ precipitates)
  • Cr–Zr composite: Superior grain refinement vs 7A52
  • Low Fe/Si: Enhances toughness
  • Trace Be: Improves castability

Core Element Roles

  • Zn: Forms high‑density η′ precipitates; main strength source
  • Mg: Synergizes with Zn for precipitation strengthening
  • Cr/Zr: Refine grains; suppress recrystallization
  • Mn: Improves formability/weldability
  • Cu: Enhances aging response
  1. Mechanical Properties

Typical Properties by Temper

Temper Tensile Strength (MPa) Yield Strength (MPa) Elongation (%) Hardness (HBW) Weldability Primary Use
T4 380–440 280–340 12–16 105–120 Good Pre‑weld components
T6 500–600+ 430–550+ 5–10 141–160 Good Armor main structure
T651 480–550 420–480 6–10 138–150 Good Thick plates
T7X 450–520 390–450 7–12 130–145 Good Corrosive environments
H112 420–480 340–400 8–12 120–135 Good Extra‑thick forgings

T6 Full‑Thickness Properties

Thickness (mm) Tensile Strength ≥ (MPa) Yield Strength ≥ (MPa) Elongation ≥ (%)
0.5–6 530–600 460–530 6–9
6–25 510–570 440–500 6–9
25–50 490–540 420–470 5–8
50–75 470–520 400–450 5–8
75–100 450–500 380–430 5–7

Physical Properties

Property Value Range
Density 2.78–2.83 g/cm³
Melting range 475–650 °C
Thermal conductivity 120–150 W/(m·K)
Elastic modulus 69–72 GPa
Poisson’s ratio 0.33
  1. Welding Performance

Methods & Parameters

  • MIG: 3–25 mm; ER5356/5A56/Sc‑wire
  • TIG: 1–10 mm; ER5356
  • FSW: 3–50 mm; no filler
  • Joint strength: ≥70 % base metal

Key Characteristics

  • Compatible with 7A52: Weldable to 7A52
  • Lower melting point: Easier preheating
  • Post‑weld aging: Restores strength

Armor Alloy Comparison

Alloy Tensile Strength Weldability Impact Behavior Primary Use
7A62 500–600 MPa Excellent Ductile + spall High‑strength armor
7A52 469–600 MPa Good Only ductile Tough armor layers
7055 580–650 MPa Very poor Brittle Aviation parts

VII. Ultrasonic Testing (UT)

Standards

  • Military: GJB 9614‑2019
  • Industrial: ASTM B594/B548

Acceptance Defects

Thickness Military Grade Industrial Grade
≤12.5 mm ≤Φ1.2 mm ≤Φ1.6 mm
12.5–100 mm ≤Φ1.6 mm ≤Φ2.0 mm
100–300 mm ≤Φ2.0 mm ≤Φ2.5 mm

VIII. Grain Size (GB/T 3246.1 / ASTM E112)

Product Thickness Grade Avg Size
Thin sheet 0.2–6 mm ≥7 ≤20 μm
Medium plate 6–100 mm ≥6 ≤30 μm
Thick plate 100–300 mm ≥5 30–50 μm
  1. Dimensional Tolerances
Thickness GB/T 3880 EN 485‑4 ASTM B209
0.2–0.6 mm ±0.03 ±0.03 ±0.03
0.6–2.0 mm ±0.10 ±0.10 ±0.10
2.0–6.0 mm ±0.25 ±0.25 ±0.25
6.0–25 mm ±0.60 ±0.60 ±0.60
25–100 mm +1.0/0 +1.0/0 +0.8/0
100–200 mm +1.2/0 +1.2/0 +1.0/0
200–300 mm +1.5/0 +1.5/0 +1.2/0
  1. Production Process

T6

Melting → degassing → homogenization → rolling/forging → solution → aging → finishing → UT

T651

Homogenization → rolling → solution → tension relief → aging → finishing

T4

Homogenization → rolling → solution → natural aging → finishing

T7X

Homogenization → rolling → solution → overaging → finishing

H112

Forging → air cool → finishing → UT

0 replies

Leave a Reply

Want to join the discussion?
Feel free to contribute!

Leave a Reply

Your email address will not be published. Required fields are marked *