7075-T651 vs T6 Aluminum: Which is Better for Your Precision Parts?
7075 is an ultra-high-strength, heat-treatable Al-Zn-Mg-Cu aluminum alloy, known as the “King of Aluminum Alloys”. It features high strength, high hardness, and excellent fatigue resistance, widely used in aerospace, military, high-end molds, racing vehicles, and premium mechanical structures.
Limitations: Moderate corrosion resistance, poor weldability, and susceptibility to stress corrosion cracking.
- Alloy Composition
Specifications: EN 573-3 / EN AW-7075 (AlZn5.5MgCu) & ASTM B209 / AMS 4049
| Element | Si | Fe | Cu | Mn | Mg | Cr | Zn | Ti | Other (Single) | Other (Total) | Al |
| Requirement (wt%) | ≤0.40 | ≤0.50 | 1.2–2.0 | ≤0.30 | 2.1–2.9 | 0.18–0.28 | 5.1–6.1 | ≤0.20 | ≤0.05 | ≤0.15 | Balance |
Key Element Functions
- Zn: Main strengthening element; forms MgZn₂ with Mg, significantly boosting strength.
- Mg: Synergizes with Zn to form strengthening phases, enhancing heat treatment response.
- Cu: Improves strength, stress corrosion resistance, and refines grain structure.
- Cr: Inhibits recrystallization, refines grains, and improves toughness and corrosion resistance.
- Thickness: 0.5–4.0 mm
Thin sheets in 0.5–4.0 mm are ideal for wing skins, door panels, precision brackets, and other structural parts requiring high rigidity and lightweighting.
Tolerance: Strictly controlled per EN 485-1:
- ≤2.0 mm: ±0.05 mm
- 0–4.0 mm: ±0.10 mm
Production Process Note:
- ≤4.0 mm: Requires air cushion furnace for heat treatment (no surface contact, zero scratches).
- >4.0 mm: Box furnace or roller hearth furnace is sufficient.
Air Cushion Furnace: A high-precision heat treatment equipment using air flotation technology. It processes aluminum/copper strips without contact, ensuring scratch-free surfaces, precise temperature control, and consistent mechanical properties. Widely used in aerospace, new energy vehicles, and premium metal processing.
- Mechanical Properties – 7075-O (Annealed)
ASTM B209 (Sheet / Plate)
| Thickness (mm) | Tensile Strength (MPa) | Yield Strength (MPa, 0.2%) | Elongation (% A50mm) |
| ≤1.5 | 220–260 | ≤100 | ≥16 |
| 1.5–3.0 | 220–260 | ≤100 | ≥15 |
| 3.0–6.0 | 220–260 | ≤100 | ≥14 |
| 6.0–12.5 | 220–260 | ≤100 | ≥13 |
| 12.5–25 | 220–260 | ≤100 | ≥12 |
| 25–50 | 220–260 | ≤100 | ≥11 |
| 50–100 | 220–260 | ≤100 | ≥10 |
| 100–200 | 220–260 | ≤100 | ≥9 |
EN 485-2 (EN AW-7075-O)
| Thickness (mm) | Tensile Strength (MPa) | Yield Strength (MPa) | Elongation (%) |
| ≤6 | 210–260 | ≤100 | ≥12 |
| 6–25 | 210–260 | ≤100 | ≥10 |
| 25–80 | 210–260 | ≤100 | ≥8 |
| 80–200 | 210–260 | ≤100 | ≥7 |
Key Feature for O-Temper:
Tensile and yield strength are nearly constant across all thicknesses, while elongation decreases as thickness increases (typical for annealed aluminum alloys).
- Mechanical Properties – 7075-T6 (Solution + Peak Aging)
Standards: ASTM B209 / EN 485
| Thickness (mm) | Tensile Strength (MPa) | Yield Strength (MPa) | Elongation (% A50mm) |
| 0.8–1.5 | ≥540 | ≥460 | ≥6 |
| 1.5–3.0 | ≥540 | ≥470 | ≥7 |
| 3.0–6.0 | ≥545 | ≥475 | ≥8 |
| 6.0–12.5 | ≥550 | ≥480 | ≥9 |
| 12.5–25 | ≥550 | ≥480 | ≥8 |
| 25–100 | ≥540 | ≥470 | ≥7 |
| 100–200 | ≥530 | ≥460 | ≥6 |
| Hardness (HBW) | 140–150 | — | — |
- Mechanical Properties – 7075-T651 (Solution + Stress Relief + Aging)
Standards: ASTM B209 / EN 485
| Thickness (mm) | Tensile Strength (MPa) | Yield Strength (MPa) | Elongation (% A50mm) |
| 0.8–1.5 | ≥540 | ≥460 | ≥6 |
| 1.5–3.0 | ≥540 | ≥470 | ≥7 |
| 3.0–6.0 | ≥545 | ≥475 | ≥8 |
| 6.0–12.5 | ≥550 | ≥480 | ≥9 |
| 12.5–25 | ≥550 | ≥480 | ≥8 |
| 25–100 | ≥540 | ≥470 | ≥7 |
| 100–200 | ≥530 | ≥460 | ≥6 |
| Hardness (HBW) | 145–160 | — | — |
- Production Process
7075-O (0.5–4.0 mm)
- Casting: Melting and refining per 7075 composition.
- Face Milling: Remove surface defects from ingots.
- Homogenization: High-temperature soaking to eliminate segregation.
- Hot Rolling: Roll to 6–10 mm intermediate thickness.
- Cold Rolling: Multiple passes to final 0.5–4.0 mm.
- O-Annealing: Medium-temperature soaking + furnace cooling for full recrystallization.
- Straightening & Cutting: Roller leveling, fixed-length shearing.
- Finishing: Polishing, film coating, marking, cutting, weighing, packaging.
- Inspection & Storage: Dimensional, mechanical, and surface checks before shipping.
7075-T6 / T651 (0.5–4.0 mm)
- Casting → Face Milling
- Homogenization
- Hot rolling to 6–10 mm
- Cold rolling to 0.5–4.0 mm
- Solution treatment + rapid water quenching
- Artificial aging (core T6 process)
- Stretching for stress relief (T651 only)
- Finishing → Inspection → Packaging
- Dimensional Tolerances
| Item | EN 485-4 (Group II) | ANSI H35.2 (Commercial) | ANSI H35.2 (Aerospace) |
| Thickness (mm) | 0.5–1.0: +0.06/–0.04
1.1–2.0: +0.07/–0.05 2.1–3.0: +0.08/–0.06 3.1–4.0: +0.10/–0.08 |
0.51–1.0: +0.0015 in
1.0–2.0: +0.0020 in 2.0–4.0: +0.0035 in |
Same as commercial, tighter overall |
| Width (mm) | Cold-rolled: +4/–0 (≤1250 mm)
+5/–0 (1251–1600 mm) |
Sheared: +3.2 mm (≤1000 mm)
+4.8 mm (1001–1500 mm) |
+1.6 mm (≤1000 mm)
+3.2 mm (1001–1500 mm) |
| Length (mm) | Cold-rolled: +6/–0 (≤3000 mm) | Sheared: +3.2 mm (≤2000 mm)
+6.4 mm (2001–3000 mm) |
+1.6 mm (≤2000 mm)
+3.2 mm (2001–3000 mm) |
| Diagonal (mm) | Ref. GB/T 3194 High Precision: ≤0.8×W/100 | Same as EN | Aerospace: ≤0.7×W/100 |
| Flatness (mm/m) | Cold-rolled: ≤10 | ≤12 | ≤6 |
Notes:
- EN 485-4: Group II, width-dependent thickness tolerance; only positive tolerances for width/length.
- ANSI H35.2: Commercial vs. Aerospace grades (aerospace tighter).
- Special sizes (cut-to-length, alclad, super flat) available with negotiated tighter tolerances.


Leave a Reply
Want to join the discussion?Feel free to contribute!