7055 Aluminum Alloy: Ultra-High Strength 7000 Series for Aerospace Wing Structures
- Material Overview
7055 is an ultra‑high‑strength, heat‑treatable, wrought aluminum alloy of the Al–Zn–Mg–Cu series. Registered as AA7055 (UNS A97055), it was developed and commercialized by Alcoa in 1991. It is among the highest‑strength commercial aluminum alloys available today. Derived from 7050, it features increased zinc and copper contents and reduced iron and silicon impurities, delivering extreme strength, good toughness, and improved stress corrosion resistance. It is widely used in aerospace structures, including the Boeing 777 and Airbus A380.
Core Advantages
- Ultra‑high strength: Tensile strength up to 600–680 MPa; yield strength ≥ 600 MPa
- Superior compressive performance: Compressive strength 7–10 % higher than 7150
- High load‑bearing capacity: 4 % stronger than traditional 2A14 alloy
- Excellent balance: Combines extreme strength with good fracture toughness and corrosion resistance
- Aerospace flagship: Optimized for high‑stress compressive structures (wing panels, spars, keel beams)
Standards Compliance
- EN 573‑3: Chemical composition
- ASTM B209: Aluminum alloy sheet and plate
- AMS 4206: 7055‑T7751 sheet
- AMS 4336: 7055‑T7651 extrusions
- AMS 4337: 7055‑T7751 extrusions
Edition Notes
This report is aligned with AA, AMS, and commercial test data. It covers 0.2 mm thin sheets to 300 mm extra‑thick forgings and includes full temper data (T6, T651, T7651, T7751, T7951) for drawing, material selection, procurement, and quality inspection.
- Full‑Thickness Quick Reference
| Thickness Range | Product Form | Recommended Temper | Typical Applications |
| 0.2–2.0 mm | Thin sheet / strip | T6, T651, T7651 | Aircraft skins, lightweight thin‑walled parts, high‑stress thin panels |
| 2.0–6.0 mm | Rolled sheet | T6, T651, T7651 | Fuselage panels, stringers, structural ribs, wing skins |
| 6.0–25 mm | Medium–thick plate | T6, T651, T7651, T7751 | Secondary aircraft structures, fuselage frames, bulkheads, stiffeners |
| 25–100 mm | Thick plate | T651, T7651, T7751, T7951 | Wing spars, ribs, spacers, landing gear supports, keel beams |
| 100–150 mm | Extra‑thick plate | T7651, T7751, T652 | Large forging billets, heavy load frames, landing gear beams |
| 150–300 mm | Extra‑thick forging | T7651, T7751, T652 | Large aircraft forgings, heavy precision molds, ultra‑high‑strength armor parts |
Aerospace & Industrial Applications
- Aircraft: Upper wing panels, spars, horizontal stabilizers, keel beams, fuselage frames
- Commercial jets: Boeing 777, Airbus A380, C919 wing trusses
- Defense: Helicopter hubs, armored vehicle components, ship deck structures
- Spacecraft: Tiangong‑2 compressor components
- Industrial: High‑strength molds, heavy‑duty structural parts
III. Heat Treatment Specifications
- Solution treatment: 465–476 °C, water quench; hold time matched to section thickness
- Annealing: 400–450 °C
- T6 (peak aging): 120 °C / 24 h; maximum strength, poor stress corrosion resistance
- T77 (patented multi‑stage overaging): Maintains ultra‑high strength with excellent SCC and exfoliation resistance
- T7651: Balanced overaging; high strength + good corrosion resistance
- T7951: Secondary aging; high strength + improved fracture toughness
- Stress relief: 5–3 % tension/compression for plates > 25 mm and large forgings
Temper Definitions (AA / ASTM / AMS)
- T6: Solution + peak aging; highest strength, poor corrosion resistance
- T651: Solution + tension stress relief + aging; thick plates/forgings
- T652: Solution + compression stress relief + aging; large forgings
- T7651: Solution + tension stress relief + balanced overaging; high strength + good corrosion
- T7751: Solution + tension stress relief + Alcoa T77 overaging; flagship temper
- T7951: Solution + tension stress relief + secondary aging; strength + toughness balance
- Chemical Composition (Mass Fraction, %)
| Element | Si | Fe | Cu | Mn | Mg | Cr | Zn | Ti | Zr | Others (Ind.) | Others (Total) | Al |
| Limit | ≤0.15 | ≤0.15 | 1.8–2.6 | ≤0.30 | 1.8–2.6 | ≤0.04 | 7.6–8.4 | ≤0.06 | 0.08–0.25 | ≤0.05 | ≤0.15 | Balance |
Key Notes
- Based on AA and AMS standards (factory acceptance basis)
- Ultra‑high Zn (7.6–8.4 %): Main driver of record strength
- High Cu (1.8–2.6 %): Boosts aging response and corrosion resistance
- Low Fe/Si (≤0.15 %): Minimizes brittle phases; improves toughness
- Zr (0.08–0.25 %): Primary grain refiner; suppresses recrystallization
- Low Cr (≤0.04 %): Preserves Zr‑based grain refinement
Core Element Roles
- Zn: Forms high‑density MgZn₂ (η′) precipitates; main strengthening phase
- Mg: Synergizes with Zn for precipitation strengthening
- Cu: Enhances grain boundary strength and corrosion resistance
- Zr: Strong grain refinement; reduces quench sensitivity
- Fe/Si: Strictly controlled to improve fracture toughness
- Mechanical Properties (Full Thickness / Full Temper)
Typical Properties by Temper
| Temper | Tensile Strength (MPa) | Yield Strength (MPa) | Elongation A₅₀ (%) | Hardness (HBW) | Stress Corrosion Resistance | Typical Application |
| T6 | 580–630 | 520–560 | 6–9 | 160–170 | Poor | Dry‑environment ultra‑high‑strength components |
| T651 | 550–600 | 510–540 | 7–10 | 158–168 | Poor | Thick plates, strength‑focused structures |
| T7651 | 530–580 | 490–530 | 8–11 | 150–160 | Good | High‑strength, moderate‑corrosion structures |
| T7751 | 590–650 | 560–620 | 8–12 | 155–165 | Excellent | Aerospace flagship temper |
| T7951 | 560–600 | 530–560 | 8–12 | 150–160 | Good | High‑toughness, fatigue‑critical structures |
Temper Selection Guidelines
- T6/T651: Strength priority; dry, controlled environments
- T7651: Balanced strength + corrosion; general high‑stress structures
- T7751: First choice for aerospace; ultra‑high strength + excellent SCC resistance
- T7951: Strength + fracture toughness; fatigue‑critical parts
- T652: Large forgings unsuitable for tension relief
T6 Full‑Thickness Properties
| Thickness (mm) | Tensile Strength ≥ (MPa) | Yield Strength ≥ (MPa) | Elongation A₅₀ ≥ (%) | Notes |
| 0.5–6 | 600 | 540 | 7 | Peak thin‑plate strength |
| 6–25 | 580 | 520 | 7 | Medium–thick plates |
| 25–75 | 560 | 500 | 6 | Thickness‑related strength drop |
| 75–100 | 540 | 480 | 6 | Recommend T651 for residual stress |
| 100–150 | Per supplier agreement | Per supplier agreement | ≥5 | Limited use; prefer T7751/T7651 |
T651 Full‑Thickness Properties
| Thickness (mm) | Tensile Strength ≥ (MPa) | Yield Strength ≥ (MPa) | Elongation A₅₀ ≥ (%) | Notes |
| 0.5–6 | 570 | 510 | 8 | Limited thin‑plate supply |
| 6–25 | 560 | 500 | 8 | Standard pre‑stretched plate |
| 25–75 | 540 | 490 | 7 | Stable post‑stress relief |
| 75–100 | 520 | 470 | 6 | Thick‑plate core grade |
| 100–150 | 500 | 450 | 6 | Supplier agreement |
T7651 Full‑Thickness Properties
| Thickness (mm) | Tensile Strength ≥ (MPa) | Yield Strength ≥ (MPa) | Elongation A₅₀ ≥ (%) | Hardness (HBW) | Data Source |
| 0.5–6 | 550 | 500 | 9 | 148–158 | Thin‑plate typical |
| 6–25 | 540 | 490 | 9 | 148–158 | Medium–thick plate |
| 25–75 | 530 | 480 | 8 | 145–155 | Thick plate |
| 75–100 | 510 | 460 | 8 | 143–153 | Commercial grade |
| 100–150 | 490 | 440 | 7 | 140–150 | Extra‑thick plate |
T7751 Full‑Thickness Properties
| Thickness (mm) | Tensile Strength ≥ (MPa) | Yield Strength ≥ (MPa) | Elongation A₅₀ ≥ (%) | Hardness (HBW) | Data Source |
| 0.5–6 | 610 | 580 | 9 | 160–170 | Thin‑plate flagship |
| 6–25 | 600 | 570 | 9 | 158–168 | Medium–thick plate |
| 25–75 | 590 | 560 | 8 | 155–165 | AMS 4206 standard |
| 75–100 | 570 | 540 | 8 | 152–162 | Commercial grade |
| 100–150 | 550 | 520 | 7 | 148–158 | Extra‑thick plate |
T7951 Full‑Thickness Properties
| Thickness (mm) | Tensile Strength ≥ (MPa) | Yield Strength ≥ (MPa) | Elongation A₅₀ ≥ (%) | Hardness (HBW) |
| 0.5–6 | 580 | 540 | 9 | 155–165 |
| 6–25 | 570 | 530 | 9 | 152–162 |
| 25–75 | 560 | 520 | 8 | 148–158 |
| 75–100 | 545 | 500 | 8 | 145–155 |
| 100–150 | 525 | 480 | 7 | 142–152 |
T652 Extra‑Thick Forging Properties
| Thickness (mm) | Tensile Strength ≥ (MPa) | Yield Strength ≥ (MPa) | Elongation A₅₀ ≥ (%) | Notes |
| 100–130 | 520 | 490 | 6 | Industry reference |
| 130–150 | 500 | 470 | 6 | Industry reference |
| 150–200 | 480 | 450 | 5 | Industry reference |
| 200–300 | 460 | 430 | 5 | Industry reference |
Physical Properties
| Property | Value Range | Notes |
| Density | 2.86 g/cm³ | AA typical |
| Melting range | 475–655 °C | Solidus ≈ 490 °C |
| Specific heat capacity | 0.860 J/(g·°C) | At 20 °C |
| Thermal conductivity | 120–155 W/(m·K) | Room temperature |
| Electrical conductivity | 18–30 % IACS | T77: 22–26 % IACS |
| Linear expansion coefficient | 23.5–24.0 × 10⁻⁶ /K | 20–100 °C |
| Elastic modulus | 70.0–72.0 GPa | Typical: 71.0 GPa |
| Shear modulus | 26.0–27.0 GPa | Typical: 26.5 GPa |
| Poisson’s ratio | 0.33 | Typical |
- Weldability & Machinability
- Weldability: Poor; fusion welding not recommended. Use bolting, riveting, or machining.
- Machinability: Good with carbide tools; excellent surface finish possible.
- Cold formability: Poor; avoid severe cold deformation.
- Corrosion: T7751/T7951 offer excellent SCC resistance; T6/T651 require protection.
VII. Ultrasonic Testing (UT)
Standards
- Aerospace: AMS‑STD‑2154, ASTM B594
- Industrial: ASTM B548
Acceptance Defect Size
| Thickness (mm) | Aerospace Grade | Industrial Grade |
| ≤12.5 | ≤Φ1.2 mm | ≤Φ1.6 mm |
| 12.5–100 | ≤Φ1.6 mm | ≤Φ2.0 mm |
| 100–300 | ≤Φ2.0 mm | ≤Φ2.5 mm |
Rejection Criteria
- Delamination, cracks, dense inclusions, large porosity, severe back‑wall attenuation
VIII. Grain Size
Standard: ASTM E112
| Product Form | Thickness | Grade | Average Size |
| Thin sheet/strip | 0.2–6 mm | ≥7 | ≤20 μm |
| Medium–thick plate | 6–100 mm | ≥6 | ≤30 μm |
| Extra‑thick forging | 100–300 mm | ≥5 | 30–50 μm |
- Dimensional Tolerances
| Thickness (mm) | EN 485‑4 | ASTM B209 | Aerospace Precision |
| 0.2–0.6 | ±0.03 | ±0.03 | ±0.020 |
| 0.6–2.0 | ±0.10 | ±0.10 | ±0.08 |
| 2.0–6.0 | ±0.25 | ±0.25 | ±0.20 |
| 6.0–25 | ±0.60 | ±0.60 | ±0.48 |
| 25–100 | +1.0 / 0 | +0.8 / 0 | +0.6 / 0 |
| 100–200 | +1.2 / 0 | +1.0 / 0 | +0.7 / 0 |
| 200–300 | +1.5 / 0 | +1.2 / 0 | +0.8 / 0 |
- Production Process
T6
Melting → degassing → homogenization → hot/cold rolling → solution quench (465–476 °C) → aging (120 °C / 24 h) → finishing → UT → inspection
T651
Homogenization → hot rolling → solution quench → tension stress relief (1.5–3 %) → aging → finishing → UT
T7751 / T7651
Melting → homogenization → hot rolling/forging → solution quench → tension stress relief → T77 overaging (T7751) → finishing → UT
T7951
Forging → solution quench → T6 aging → secondary aging → tension stress relief → finishing → UT


Leave a Reply