7017 vs 7039 Aluminum: Better Stress Corrosion Resistance for Armor
1. Material Overview
7017 is an Al-Zn-Mg low‑copper, medium‑to‑high strength heat‑treatable wrought aluminum alloy. It offers an outstanding strength‑to‑weight ratio, good toughness, and superior resistance to stress corrosion cracking (SCC) and exfoliation corrosion. Widely recognized as one of the most weldable grades in the 7000 series, 7017 is ideal for demanding structural and military applications.
Compared to 7039 aluminum alloy, 7017 provides higher SCC resistance and lower susceptibility to spalling cracking, making it preferred for military armor. Its corrosion performance also exceeds conventional 5xxx alloys such as 5083 and 5039.
Typical uses include military armored vehicles, aerospace structural components, lightweight tactical bridges, and high‑strength welded structures. The alloy fully meets MIL‑DTL‑32505, which covers weldable armor aluminum plates from 12.7 mm to 101.6 mm (0.500–4.000 inches).
2. Full Thickness Application Quick Reference
| Thickness Range | Product Form | Recommended Temper | Typical Application |
| 0.1–2.0 mm | Sheet / Coil | T6, T651 | Military body skin, lightweight covers, electronic enclosures |
| 2.0–6.0 mm | Standard Plate | T6, T651 | Structural frames, connection plates, armor liners |
| 6.0–25 mm | Medium Plate | T6, T651, T7351, T7651 | Primary load‑bearing structures, armor plate, mold bases |
| 25–100 mm | Heavy Plate | T6, T651, T7351, T7651 | Heavy armor, aerospace main frames, forging billets |
| 100–150 mm | Ultra‑Heavy Plate | T651, T652, T7351 | Extra‑thick armor, large forgings, heavy equipment frames |
| 150–300 mm | Ultra‑Heavy Plate / Forging | T652 (Compression Stress Relieved) | Large military forgings, heavy die blocks, special load‑bearing structures |
Heat Treatment Characteristics
- Solution treatment temperature: 455–475°C, optimized for section thickness
- T6 peak aging delivers maximum tensile strength
- T7X overaging reduces tensile strength by 8–12% while significantly improving SCC and exfoliation corrosion resistance
- Plates thicker than 25 mm require stress relief to minimize machining distortion
Temper Definitions (AA / ASTM Standard)
- T6: Solution heat treatment + artificial peak aging
- T651: T6 + 5–3.0% cold stretching for residual stress relief
- T652: T6 + stress relief via controlled compression (1–5% permanent set), for thick plates and large forgings
- T7351: Solution treatment + stretch stress relief + stabilized overaging (maximum SCC resistance)
- T7651: Solution treatment + stretch stress relief + intermediate overaging (balanced strength and exfoliation resistance)
3. Chemical Composition (Mass Fraction %)
Table 1: 7017 Aluminum Alloy Chemical Composition (EN 573‑3 / AA Standard)
| Element | Si | Fe | Cu | Mn | Mg | Cr | Zn | Ti | Zr | Others (Single) | Others (Total) | Al |
| Limit | ≤0.35 | ≤0.45 | ≤0.20 | 0.05–0.50 | 2.0–3.0 | ≤0.035 | 4.0–5.2 | ≤0.15 | 0.10–0.25 | ≤0.05 | ≤0.15 | Remainder |
Important Notes
- Values comply with EN 573‑3 and AA standards and are the sole basis for engineering acceptance.
- Some commercial datasheets list non‑standard ranges (Zn: 5.8–6.8%, Cu: 0.8–1.5%, Cr: 0.08–0.16%). These are modified non‑standard alloys and cannot replace 7017.
- All mechanical and corrosion data in this report strictly follow EN 573‑3 standard composition.
Functions of Major Alloying Elements
- Zn + Mg: Form MgZn₂ (η’) strengthening precipitates for primary age hardening
- Mg: Enhances strength and improves aging response
- Mn: Refines grain structure, raises recrystallization temperature, stabilizes microstructure
- Cr: Restricts grain boundary coarsening; works with Mn to control grain size
- Zr: Forms Al₃Zr dispersoids to inhibit recrystallization, refine grains, and boost SCC resistance
- Low Cu (≤0.20%): Reduces copper‑rich grain boundary precipitates, greatly improving weldability and stress corrosion performance — a key advantage over 7075 (Cu: 1.2–2.0%).
4. Mechanical Properties (Full Thickness & All Tempers)
4.1 Data Classification
- Standard Specification Data: EN 485, ASTM B209, MIL‑DTL‑32505 (authoritative for acceptance)
- Typical Commercial Data: Authorized mill TDS (for design reference only)
- Academic Literature Data: Journal experimental results (research only, not for engineering acceptance)
4.2 Overall Mechanical Property Summary
Table 2: Typical Mechanical Properties of 7017 by Temper
| Temper | Tensile Strength Rm (MPa) | Yield Strength Rp₀.₂ (MPa) | Elongation A₅₀ (%) | Hardness HBW | SCC Resistance |
| T6 | 560–605 | 490–535 | 9–13 | 150–160 | Moderate |
| T651 | 570–615 | 500–545 | 8–12 | 153–163 | Moderate |
| T7351 | 455–490 | 385–420 | 10–14 | 130–140 | Excellent |
| T7651 | 485–525 | 425–465 | 9–12 | 140–152 | Good |
Temper Selection Guide
- T6 / T651: Maximum strength; not recommended for severe corrosion or long‑term SCC environments
- T7351: First choice for marine, salt spray, and high‑humidity service requiring superior SCC performance
- T7651: Optimal balance of strength and exfoliation corrosion resistance
- T651 unavailable below 0.5 mm (process limit); T652 for ultra‑thick plates and forgings only
4.3 T6 Temper Mechanical Properties
Table 3: 7017‑T6 Mechanical Properties
| Thickness (mm) | Min Rm (MPa) | Min Rp₀.₂ (MPa) | Min A₅₀ (%) | HBW Range | Data Source |
| 0.5–6 | 530 | 460 | 7 | 145–160 | ASTM B209 / MIL‑DTL‑32505 |
| 6–25 | 520 | 450 | 7 | 145–160 | Standard / Mill TDS |
| 25–75 | 510 | 440 | 7 | 140–155 | Commercial database |
| 75–100 | 490 | 420 | 6 | 135–150 | Commercial database |
| 100–150 | 470 | 400 | 6 | 130–150 | Thickness effect interpolation |
4.4 T651 Temper Mechanical Properties
Table 4: 7017‑T651 Mechanical Properties
| Thickness (mm) | Min Rm (MPa) | Min Rp₀.₂ (MPa) | Min A₅₀ (%) | HBW Range |
| 0.5–6 | 540 | 470 | 7 | 153–163 |
| 6–25 | 530 | 460 | 7 | 150–160 |
| 25–75 | 520 | 450 | 7 | 148–160 |
| 75–100 | 500 | 430 | 6 | 145–158 |
| 100–150 | 470 | 400 | 6 | 140–155 |
4.5 T7351 Temper Mechanical Properties
Table 5: 7017‑T7351 Mechanical Properties
| Thickness (mm) | Min Rm (MPa) | Min Rp₀.₂ (MPa) | Min A₅₀ (%) | HBW Range |
| 0.5–6 | 460 | 390 | 8 | 130–140 |
| 6–25 | 455 | 385 | 8 | 128–140 |
| 25–75 | 445 | 375 | 8 | 125–138 |
| 75–100 | 435 | 365 | 7 | 120–135 |
| 100–150 | 425 | 355 | 7 | 115–130 |
4.6 T7651 Temper Mechanical Properties
Table 6: 7017‑T7651 Mechanical Properties
| Thickness (mm) | Min Rm (MPa) | Min Rp₀.₂ (MPa) | Min A₅₀ (%) | HBW Range |
| 0.5–6 | 500 | 430 | 7 | 140–152 |
| 6–25 | 490 | 420 | 7 | 138–150 |
| 25–75 | 480 | 410 | 7 | 135–148 |
| 75–100 | 470 | 400 | 6 | 130–145 |
| 100–150 | 460 | 390 | 6 | 125–140 |
4.7 T652 Temper Mechanical Properties (Ultra‑Heavy Plate / Forging)
Table 7: 7017‑T652 Mechanical Properties
| Thickness (mm) | Min Rm (MPa) | Min Rp₀.₂ (MPa) | Min A₅₀ (%) |
| 100–130 | 450 | 380 | 6 |
| 130–150 | 440 | 370 | 6 |
| 150–200 | 430 | 360 | 5 |
| 200–300 | 420 | 350 | 5 |
Important Statement
- ASTM B247M does not formally list 7017 (A97017); no mandatory standard mechanical values exist.
- Data are interpolated per 7xxx thickness attenuation rules and 7017 performance trends (design reference only).
- Procurement and engineering acceptance require mill test certificates, tensile test reports, and ultrasonic inspection records.
4.8 Physical Properties (All Tempers)
Table 8: Typical Physical Properties of 7017 Aluminum Alloy
| Property | Metric | Imperial |
| Density | 2.81 g/cm³ | 0.101 lb/in³ |
| Melting Range | 475–635°C | 887–1175°F |
| Electrical Conductivity (T6) | 34–38% IACS | 34–38% IACS |
| Thermal Conductivity | 138–153 W/m·K | 955–1060 BTU·in/(hr·ft²·°F) |
| Coefficient of Thermal Expansion | 23.6×10⁻⁶/K | 13.1×10⁻⁶/°F |
| Modulus of Elasticity | 71 GPa | 10300 ksi |
| Shear Modulus | 27 GPa | 3920 ksi |
5. MIL‑DTL‑32505 Armor Plate Specification
5.1 Thickness Coverage
Nominal thickness: 0.500–4.000 inches (12.7–101.6 mm)
5.2 Material Class
- Class I: 7017 alloy, superior SCC resistance for welded and non‑welded armor
- Class II: 7020 alloy
5.3 Referenced Standards
ASTM B557, SAE AMS 2750, ASTM E716, MIL‑STD‑662 (V50 ballistic test method)
6. Ultrasonic Testing (UT) Standard
6.1 Applicable Standards
- Aerospace Grade: ASTM B594
- General Structural Grade: ASTM B548
6.2 Testing Parameters
| Parameter | Requirement |
| Probe | 2.5 MHz, Φ20 mm straight probe |
| Reference Sensitivity | Φ1.2 mm flat‑bottom hole, DAC curve evaluation |
| Scanning | 100% full surface coverage, overlap ≥10% |
6.3 Acceptance Level
Table 9: UT Acceptance Criteria (ASTM B594)
| Thickness (mm) | Max Defect Equivalent (Aerospace Grade) | Max Defect Equivalent (General Grade) |
| 0.5–12.5 | ≤Φ1.2 mm | ≤Φ1.6 mm |
| 12.5–100 | ≤Φ1.6 mm | ≤Φ2.0 mm |
| 100–150 | ≤Φ1.6 mm | ≤Φ2.0 mm |
| 150–300 | ≤Φ2.0 mm | ≤Φ2.5 mm |
6.4 Rejection Criteria
- Signal amplitude exceeding DAC +2 dB
- Cracks, porosity, clustered inclusions, or delaminations
- Back wall echo loss >80%
7. Grain Size Standard
7.1 Standard
ASTM E112 (intercept or comparison method); specimens taken at 1/2 thickness transverse section.
7.2 Grain Size Requirements
Table 10: 7017 Aluminum Alloy Grain Grade
| Product Form | Thickness (mm) | Minimum Grain Size Grade | Average Grain Size |
| Sheet / Plate | 0.1–6 | Grade 7 | ≤15 μm |
| Medium / Heavy Plate | 6–100 | Grade 6 | ≤25 μm |
| Ultra‑Heavy Plate / Forging | 100–300 | Grade 5 | 25–50 μm |
7.3 Inspection Procedure
Mounting → Grinding → Polishing → Etching (Keller’s Reagent) → Microscopy (100×/200×) → Grain sizing per ASTM E112
8. Dimensional Tolerances (Full Thickness)
Table 11: Thickness Tolerances (EN 485‑4 / ASTM H35.2)
| Thickness (mm) | EN 485‑4 | Commercial Grade | Aerospace Grade |
| 0.1–0.2 | ±0.015 | ±0.015 | ±0.01 |
| 0.2–0.4 | ±0.02 | ±0.02 | ±0.015 |
| 0.4–0.6 | ±0.03 | ±0.03 | ±0.02 |
| 0.6–0.8 | ±0.04 | ±0.04 | ±0.03 |
| 0.8–1.0 | ±0.05 | ±0.05 | ±0.04 |
| 1.0–1.2 | ±0.06 | ±0.06 | ±0.05 |
| 1.2–1.6 | ±0.08 | ±0.08 | ±0.06 |
| 1.6–2.0 | ±0.10 | ±0.10 | ±0.08 |
| 2.0–2.5 | ±0.12 | ±0.12 | ±0.10 |
| 2.5–3.0 | ±0.15 | ±0.15 | ±0.12 |
| 3.0–4.0 | ±0.20 | ±0.20 | ±0.15 |
| 4.0–6.0 | ±0.25 | ±0.25 | ±0.20 |
| 6.0–10.0 | ±0.35 | ±0.35 | ±0.28 |
| 10.0–15.0 | ±0.45 | ±0.45 | ±0.36 |
| 15.0–25.0 | ±0.60 | ±0.60 | ±0.48 |
| 25.0–300 | +1.0 / –0 | +0.8 / –0 | +0.6 / –0 |
9. Manufacturing Process Flow
9.1 7017‑T6
Melting & Casting → Degassing & Purification → Homogenization → Hot / Cold Rolling → Solution Treatment & Water Quenching → Peak Aging → Straightening → Cutting → UT Inspection → Final Acceptance
9.2 7017‑T651
Melting & Casting → Homogenization → Hot / Cold Rolling → Solution & Quench → Stretch Stress Relief → Artificial Aging → Straightening → UT Inspection → Acceptance
9.3 7017‑T7351 / T7651
Melting & Casting → Homogenization → Rolling → Solution & Quench → Stretch Stress Relief → Controlled Overaging → Straightening → UT Inspection → Acceptance
9.4 7017‑T652 (Forging / Ultra‑Heavy Plate)
Forging / Rolling → Solution & Quench → Compression Stress Relief → Artificial Aging → Straightening → UT Inspection → Acceptance
10. Weldability & Application Summary
10.1 Welding Performance
7017 is one of the most weldable alloys in the 7000 series. It can be dissimilarly welded with 5xxx grades (e.g., 5083, 5059). Suitable for MIG, TIG, and friction stir welding (FSW). Weld joints offer high strength and good natural aging recovery in the heat‑affected zone.
10.2 Ballistic Performance
7017 aluminum plates provide excellent ballistic resistance against 7.62 mm projectiles. Peak‑aged tempers deliver maximum hardness and ballistic protection, fully meeting MIL‑DTL‑32505 V50 ballistic test requirements.
10.3 Stress Corrosion Behavior
7017 inherently outperforms 7039 in SCC resistance. T7351 and T7651 overaging tempers modify grain boundary precipitation, effectively suppressing stress corrosion cracking under sustained load and corrosive environments.


Leave a Reply
Want to join the discussion?Feel free to contribute!