- Material Overview
2219 is an Al–Cu heat-treatable high-strength aluminum alloy. Registered by the Aluminum Association (AA) as 2219 (UNS A92219), it corresponds to China’s 2219 (formerly LY19) and ISO’s AlCu6Mn. Copper is the main alloying element, with trace additions of manganese, zirconium, vanadium, and titanium. It achieves high strength, excellent elevated-temperature mechanical properties, and good weldability via complex precipitation strengthening, performing well at temperatures up to 315 °C.
Core Advantages
- High specific strength; good mechanical properties at both cryogenic and elevated temperatures
- High fracture toughness and good stress corrosion resistance
- Best weldability among 2000-series alloys; mature wire specifications
- Main structural material for rocket propellant tanks
- Maintains excellent mechanical properties from −269 °C to 315 °C
- Typical strength:
- T851: Tensile strength > 455 MPa, yield strength > 350 MPa
- T87: Tensile strength up to 476 MPa
Standards Compliance
- GB/T 3190-2020: Chemical Composition of Wrought Aluminum and Aluminum Alloys
- ASTM B209: Aluminum Alloy Sheet and Plate
- AMS 4031 / AMS 4066: Aerospace-grade specifications
- GJB 1137A-2018: 2219 Aluminum Alloy Extruded Bars for Aerospace
Edition Notes
This report aligns with GB/T 3190, AMS, ASTM, and commercial test data. It covers 0.2 mm thin sheets to 300 mm extra-thick forgings and includes full temper data (T6, T851, T87, T62, O) for drawing, material selection, procurement, and quality inspection.
- Full-Thickness Quick Reference
| Thickness Range | Product Form | Recommended Temper | Typical Applications |
| 0.2–2.0 mm | Thin sheet / strip | T6, T62, O | Supersonic aircraft skins, tank liners, thin-walled structures |
| 2.0–6.0 mm | Rolled sheet | T6, T62, T87 | Spacecraft bulkheads, aircraft skins, fuselage frames |
| 6.0–25 mm | Medium–thick plate | T6, T851, T87 | Rocket tank shells, liquid oxygen tanks, welded structures |
| 25–100 mm | Thick plate | T6, T851, T87 | Rocket tank transition rings, missile casings, engine frames |
| 100–150 mm | Extra-thick plate / ring | T851, T852 | Large-diameter tank rings, heavy rocket thrust structures |
| 150–300 mm | Extra-thick ring / forging | T851, T852 | Ultra-large integral rings, major aerospace load-bearing components |
Aerospace Applications
- Zhongke Lijian-2 launch vehicle: Second-stage tank (first domestic large-diameter smooth cylindrical tank)
- Long March series: Tank structures, 5 m diameter integral rings (Long March 5B), fuel tanks (Long March 9)
- Reusable liquid oxygen tanks: Primary material due to excellent weldability
- Supersonic aircraft: Skins and structural components
III. Heat Treatment Specifications
- Solution treatment: 530–540 °C, water quench; typical: 535 °C / 45 min
- T6 (peak aging): Forgings: 190 °C / 18 h; sheets: 190 °C / 36 h
- T851 / T87: Solution → 5–8 % cold work → artificial aging (T87: highest strength)
- T62: Solution by user → aging by manufacturer (for formed parts)
- O (annealed): Maximum plasticity, for deep drawing
- Extra-thick products: Stress relief via T851 (tensile) or T852 (compressive)
Temper Definitions (AA / ASTM / AMS)
- O: Annealed; min strength, max plasticity
- T6: Solution + peak aging (no stress relief)
- T62: Solution (user) + aging (manufacturer)
- T81 / T851: Solution → tensile stress relief → cold work → aging
- T852: Solution → compressive stress relief → aging (for ultra-thick rings/forgings)
- T87: Solution → 5–8 % cold work → aging (max strength)
- T351 / T352: Solution → stress relief → natural aging
- Chemical Composition (Mass Fraction, %)
| Element | Si | Fe | Cu | Mn | Mg | Cr | Zn | Ti | Zr | V | Others (Ind.) | Others (Total) | Al |
| Limit | ≤0.20 | ≤0.30 | 5.8–6.8 | 0.20–0.40 | ≤0.02 | — | ≤0.10 | 0.02–0.10 | 0.10–0.25 | 0.05–0.15 | ≤0.05 | ≤0.15 | Balance |
Key Notes
- Based on GB/T 3190-2020 and AA standards (factory acceptance basis)
- High Cu (5.8–6.8 %): Core of high strength and elevated-temperature performance
- Zr (0.10–0.25 %): Forms Al₃Zr dispersoids; inhibits recrystallization, improves thermal stability
- V + Mn: Enhance matrix strength at room and elevated temperatures
- Low Fe/Si: Reduces brittle phases; improves weldability and fracture toughness
- Low Mg (≤0.02 %): Distinct from Al–Mg/Al–Zn–Mg alloys
Core Element Roles
- Cu: Forms θ′(Al₂Cu) precipitates; main strengthening phase
- Mn: Improves rolling formability; grain growth inhibition
- Zr: Primary grain refiner; key difference vs other Al–Cu alloys
- V: Boosts aging response; multi-element dispersion strengthening
- Ti: Assists grain refinement
- Fe/Si: Strictly controlled for weldability and toughness
- Mechanical Properties (Full Thickness / Full Temper)
Typical Properties by Temper
| Temper | Tensile Strength (MPa) | Yield Strength (MPa) | Elongation A₅₀ (%) | Hardness (HBW) | Stress Corrosion Resistance | Typical Application |
| O | 170–220 | 70–120 | 14–18 | 60–70 | Excellent | Deep drawing, cold-work substrates |
| T6 | 365–420 | 240–290 | 8–12 | 115–125 | Good | General structural parts |
| T62 | 415–450 | 290–330 | 10–12 | 120–130 | Good | Post-forming aging components |
| T81/T851 | 455–476 | 350–380 | 8–10 | 135–145 | Good | Aerospace tank core temper |
| T87 | 476–490 | 380–395 | 8–10 | 140–150 | Good | Highest-strength structural parts |
| T351 | 380–420 | 270–320 | 10–14 | — | Good | Naturally aged stabilized parts |
Temper Selection Guidelines
- T6: General strength, non-welded components
- T62: Formed/welded parts requiring post-manufacture aging
- T851: Preferred for aerospace tank welded structures (25 mm+)
- T87: Maximum strength requirements
- T852: Ultra-thick rings/forgings (AMS 4144G)
- O: Deep drawing and heavy forming
T6 Full-Thickness Properties
| Thickness (mm) | Tensile Strength ≥ (MPa) | Yield Strength ≥ (MPa) | Elongation A₅₀ ≥ (%) | Notes |
| 0.5–6 | 400 | 280 | 8 | Thin/medium plates |
| 6–25 | 380 | 260 | 8 | Medium–thick plates |
| 25–75 | 365 | 250 | 6 | Thick plates |
| 75–100 | 365 | 240 | 6 | ASTM B209 requirements |
| 100–150 | Per supplier agreement | Per supplier agreement | ≥5 | Limited use; prefer T851 |
T851 Full-Thickness Properties
| Thickness (mm) | Tensile Strength ≥ (MPa) | Yield Strength ≥ (MPa) | Elongation A₅₀ ≥ (%) | Notes |
| 0.5–6 | 455 | 350 | 8 | Thin/medium plates |
| 6–25 | 455 | 350 | 8 | Primary tank structure |
| 25–75 | 455 | 350 | 7 | Thick plates |
| 75–100 | 450 | 345 | 6 | Extra-thick plates |
| 100–150 | 440 | 335 | 6 | Supplier agreement |
T87 Full-Thickness Properties
| Thickness (mm) | Tensile Strength ≥ (MPa) | Yield Strength ≥ (MPa) | Elongation A₅₀ ≥ (%) | Notes |
| 0.5–6 | 476 | 380 | 8 | Sheet maximum strength |
| 6–25 | 476 | 385 | 8 | Medium–thick plates |
| 25–75 | 470 | 380 | 7 | Thick plates |
| 75–100 | 465 | 375 | 7 | Extra-thick plates |
Physical Properties
| Property | Value Range | Notes |
| Density | 2.84–2.85 g/cm³ | Typical AA: 2.84 g/cm³ |
| Melting range | 543–643 °C | Solidus: 543 °C; liquidus: 643 °C |
| Solution temperature | 530–540 °C | Standard practice |
| Specific heat capacity | 860–870 J/(kg·K) | At 20 °C |
| Thermal conductivity | 110–170 W/(m·K) | Room temperature; temper-dependent |
| Electrical conductivity | 26–32 % IACS | Room temperature |
| Resistivity | 3.9–6.2 × 10⁻⁸ Ω·m | Room temperature |
| Linear expansion coefficient | 22.0–22.3 × 10⁻⁶ /K | 20–100 °C |
| Elastic modulus | 70–73 GPa | AA typical |
| Shear modulus | 26–27 GPa | Typical |
| Poisson’s ratio | 0.33 | Typical |
- Welding Performance & Material Selection
Weldability
- Best among 2000-series Al–Cu alloys
- Methods: TIG, MIG, VPPA, FSW (friction stir welding)
- Preferred filler: ER2319 (Al–Cu); ER5087 (Al–Mg) optional
- Joint strength coefficient: 63–72 % of base metal; post-weld aging → 6 %+
Welding Parameters
| Method | Thickness | Wire | Post-Weld Treatment | Application |
| TIG/GTAW | 1–10 mm | ER2319 | Artificial aging | Tank heads, connecting rings |
| MIG/GMAW | 3–20 mm | ER2319 / custom | Artificial aging | Tank longitudinal/circumferential seams |
| VPPA | 6–25 mm | ER2319 | Artificial aging | Large-diameter tank high-efficiency welding |
| FSW | 3–50 mm | None | Artificial aging | Tank main structure preferred |
Key Welding Considerations
- Control heat input to avoid HAZ overaging
- Remove oxide film and oil before welding
- Interpass temperature < 150 °C
- Dry ER2319 wire to reduce porosity
- Symmetrical welding sequence to minimize distortion
- Weld fusion line: lowest corrosion resistance → post-weld protection required
Material Selection vs. 2A14 / 7-Series
| Comparison | 2219 | 2A14 | 7050/7055 | 7A52/7A62 |
| Alloy system | Al–Cu | Al–Cu–Mg–Si | Al–Zn–Mg–Cu | Al–Zn–Mg |
| Weldability | Excellent | Good | Poor–very poor | Good |
| Elevated temp (315 °C) | Excellent | Moderate | Moderate | Moderate |
| Cryogenic (−253 °C) | Excellent | Good | Good | Good |
| Fracture toughness | 35–40 MPa·√m | 25–30 MPa·√m | 22–35 MPa·√m | Good |
| Primary use | Rocket tanks, cryogenic structures | Aircraft frames, early tanks | Non-welded aerospace structures | Armored vehicle weldments |
Conclusion
- Rocket propellant tanks: 2219 (optimal balance of cryogenic/elevated temp performance + weldability + toughness)
- Ultra-low temperature (LOX/LH₂ tanks): 2219
VII. Ultrasonic Testing (UT)
Standards
- Aerospace: ASTM B594, AMS-STD-2154, AMS 4144G
- Industrial: ASTM B548
Acceptance Defect Size
| Thickness (mm) | Aerospace Grade | Industrial Grade |
| ≤12.5 | ≤Φ1.2 mm | ≤Φ1.6 mm |
| 12.5–100 | ≤Φ1.6 mm | ≤Φ2.0 mm |
| 100–300 | ≤Φ2.0 mm | ≤Φ2.5 mm |
Rejection Criteria
- Delamination, cracks, dense inclusions, large porosity, severe back-wall attenuation
VIII. Grain Size
Standard: ASTM E112 / GB/T 3246.1
| Product Form | Thickness | Grade | Average Size |
| Thin sheet/strip | 0.2–6 mm | ≥7 | ≤20 μm |
| Medium–thick plate | 6–100 mm | ≥6 | ≤30 μm |
| Extra-thick plate/ring | 100–300 mm | ≥5 | 30–50 μm |
Note
Zr additions (Al₃Zr) strongly inhibit recrystallization → excellent grain size uniformity in thick sections.
- Dimensional Tolerances
| Thickness (mm) | GB/T 3880 | EN 485-4 | ASTM B209 | Aerospace Precision |
| 0.2–0.6 | ±0.03 | ±0.03 | ±0.03 | ±0.020 |
| 0.6–2.0 | ±0.10 | ±0.10 | ±0.10 | ±0.08 |
| 2.0–6.0 | ±0.25 | ±0.25 | ±0.25 | ±0.20 |
| 6.0–25 | ±0.60 | ±0.60 | ±0.60 | ±0.48 |
| 25–100 | +1.0 / 0 | +1.0 / 0 | +0.8 / 0 | +0.6 / 0 |
| 100–200 | +1.2 / 0 | +1.2 / 0 | +1.0 / 0 | +0.7 / 0 |
| 200–300 | +1.5 / 0 | +1.5 / 0 | +1.2 / 0 | +0.8 / 0 |
- Production Process
T6
Ingot melting → degassing → homogenization → hot/cold rolling → solution quench (535 °C) → aging (190 °C) → finishing → UT → inspection
T851
Homogenization → hot rolling → solution quench → tensile stress relief (1.5–3 %) → cold work → aging → UT
T87
Melting → homogenization → rolling/forging → solution quench → cold work (5–8 %) → aging → UT
T852 (Extra-thick rings/forgings)
Billet heating → forging/ring rolling → solution quench → compressive stress relief → aging → UT