2024 vs 7075 Aluminum: Which is Better for High-Temperature & Fatigue?
- Material Overview
2024 aluminum alloy is a heat‑treatable Al‑Cu‑Mg wrought alloy, the most widely used grade in the 2xxx series. It delivers high strength, excellent fatigue resistance, and superior high‑temperature performance (retains strength above 125°C, outperforming 7075).
- Thickness coverage: 3 mm to 300 mm (sheet, plate, heavy plate, ultra‑heavy plate)
- Key tempers: O, T3, T351, T4, T42, T6, T651, T62, T81, T851, T861, T72, H112
- Standards: ASTM B209, EN 485, AMS 4037, AMS 4467, GB/T 3880
- Limitations: Moderate corrosion resistance (requires cladding/anodization); susceptible to weld cracking (prefer riveting/bolting)
Typical applications: Aircraft skins, wing panels, fuselage structures, aerospace bulkheads, heavy equipment frames, mold bases, high‑load structural components.
- Chemical Composition (Mass Fraction, %)
Compliant with EN 573‑3, ASTM B209, GB/T 3190‑2022; AMS 4037 tightens Fe for aerospace grades.
| Element | Si | Fe | Cu | Mn | Mg | Cr | Zn | Ti | Others (Single) | Others (Total) | Al |
| Standard | ≤0.50 | ≤0.50 | 3.8–4.9 | 0.30–0.90 | 1.2–1.8 | ≤0.10 | ≤0.25 | ≤0.15 | ≤0.05 | ≤0.15 | Remainder |
| AMS 4037 | ≤0.50 | ≤0.30 | 3.8–4.9 | 0.30–0.90 | 1.2–1.8 | ≤0.10 | ≤0.25 | ≤0.15 | ≤0.05 | ≤0.15 | Remainder |
Key element roles:
- Cu: Primary strengthener (Al₂Cu, Al₂CuMg precipitates)
- Mg: Synergizes with Cu for age hardening
- Mn: Refines grains, improves toughness and exfoliation resistance
- Cr: Inhibits recrystallization, stabilizes microstructure
- Thickness Ranges & Available Tempers
3.1 Sheet: 0.3–4.0 mm
Tempers: O, T3, T4, T42, T6, T62, T81, T861
Features: Air‑furnace solution treatment (scratch‑free, uniform properties)
Uses: Aircraft skins, thin‑wall structures, precision brackets
3.2 Medium Plate: 4.5–150 mm
Tempers: O, T3, T351, T4, T42, T6, T651, T62, T81, T851, T861, T72, H112
Features: Hot rolling + batch heat treatment; T351/T651/T851 with 1–3% stretch stress relief (low distortion)
Uses: Wing spars, bulkheads, heavy equipment frames, mold bases
3.3 Ultra‑Heavy Plate: 150–300 mm
Tempers: T651 (150–200 mm), T851 (150–200 mm), T652 (150–300 mm), H112 (150–300 mm)
Features: Reduced core hardenability; T652 uses compression stress relief (max stability)
Uses: Large aerospace forgings, heavy die blocks, high‑load structures
- Mechanical Properties
4.1 Sheet (0.3–4.0 mm)
| Temper | Tensile (MPa) | Yield (MPa) | Elongation (A50, %) | Hardness (HBW) |
| O | ≤220 | ≤140 | ≥12 | 40–43 |
| T3 | ≥435 | ≥290 | ≥12 | 120 |
| T4 | ≥425 | ≥275 | ≥12 | 120–145 |
| T6 | ≥415 | ≥265 | ≥10 | 120–145 |
| T42 | ≥425 | ≥275 | ≥12 | 120–140 |
| T62 | ≥427 | ≥336 | ≥5 | 130 |
| T81 | ≥450 | ≥385 | ≥5 | 128 |
| T861 | ≥490 | ≥430 | ≥6 | 135–142 |
4.2 Medium Plate (4.5–150 mm)
| Temper | Tensile (MPa) | Yield (MPa) | Elongation (A50, %) | Hardness (HBW) |
| O | ≤220 | ≤140 | ≥8–12 | 40–43 |
| H112 | ≥380 | ≥250 | ≥10 | 80–95 |
| T3/T351 | ≥385–440 | ≥260–290 | ≥4–14 | 120 |
| T4 | ≥380–425 | ≥260–275 | ≥6–14 | 125–140 |
| T6/T651 | ≥400–460 | ≥320–380 | ≥4–9 | 125–140 |
| T81/T851 | ≥420–455 | ≥350–385 | ≥4–6 | 128–135 |
| T861 | ≥470–490 | ≥410–430 | ≥5–6 | 135–142 |
| T72 | ≥400 | ≥320 | ≥8 | 110–125 |
4.3 Ultra‑Heavy Plate (150–300 mm)
| Temper | Thickness (mm) | Tensile (MPa) | Yield (MPa) | Elongation (A50, %) | Hardness (HBW) |
| T651 | 150–200 | ≥390 | ≥305 | ≥4 | 120–145 |
| T851 | 150–200 | ≥400 | ≥330 | ≥4 | 128–135 |
| T652 | 150–200 | ≥360 | ≥280 | ≥4 | 110–130 |
| T652 | 200–250 | ≥350 | ≥270 | ≥4 | 110–130 |
| T652 | 250–300 | ≥340 | ≥260 | ≥3.5 | 110–130 |
| H112 | 150–300 | ≥350 | ≥220 | ≥8 | 80–95 |
- Physical Properties (All Tempers)
| Property | Metric | Imperial |
| Density | 2.78 g/cm³ | 0.100 lb/in³ |
| Melting Range | 500–638°C | 932–1180°F |
| Elastic Modulus | 72.4 GPa | 10500 ksi |
| Shear Modulus | 27 GPa | 3920 ksi |
| Thermal Conductivity | 121–145 W/m·K | 840–1000 BTU·in/(hr·ft²·°F) |
| CTE (20–100°C) | 22.9–23.5×10⁻⁶/K | 12.7–13.1×10⁻⁶/°F |
| Electrical Conductivity | 30–40% IACS | 30–40% IACS |
- Dimensional Tolerances (Plus Tolerance Only)
6.1 Sheet (0.3–4.0 mm)
| Thickness (mm) | EN 485‑4 | Commercial | Aerospace |
| 0.3–1.0 | +0.06 | +0.04 | +0.04 |
| 1.1–2.0 | +0.07 | +0.05 | +0.05 |
| 2.1–3.0 | +0.08 | +0.07 | +0.07 |
| 3.1–4.0 | +0.10 | +0.09 | +0.09 |
6.2 Medium Plate (4.5–150 mm)
| Thickness (mm) | EN 485‑4 | Commercial | Aerospace |
| 5–10 | +0.30 | +0.25 | +0.20 |
| 10–25 | +0.40 | +0.30 | +0.25 |
| 25–50 | +0.50 | +0.40 | +0.30 |
| 50–100 | +0.80 | +0.60 | +0.45 |
| 100–150 | +1.0 | +0.80 | +0.60 |
6.3 Ultra‑Heavy Plate (150–300 mm)
| Thickness (mm) | EN 485‑4 | Commercial | Aerospace |
| 150–200 | +1.2 | +1.0 | +0.7 |
| 200–300 | +1.5 | +1.2 | +0.8 |
- Ultrasonic Testing (UT)
- Aerospace Grade: ASTM B594
- Structural Grade: GB/T 6519 / ASTM B548
| Thickness (mm) | Aerospace Max Defect | Structural Max Defect |
| 0.3–12.5 | ≤Φ1.2 mm | ≤Φ1.6 mm |
| 12.5–150 | ≤Φ1.6 mm | ≤Φ2.0 mm |
| 150–300 | ≤Φ2.0 mm | ≤Φ3.0 mm |
Rejection criteria: Cracks, porosity, clustered inclusions; back‑wall echo loss >50%.
- Manufacturing Process Flow
8.1 Sheet (0.3–4.0 mm)
Melting → Casting → Homogenization → Hot/Cold Rolling → Air‑furnace Solution + Quench → Aging → Straightening → Shearing → Inspection
8.2 Medium Plate (4.5–150 mm)
Melting → Casting → Homogenization → Hot Rolling → Solution + Quench → Stretch Stress Relief (T351/T651/T851) → Aging → UT → Cutting
8.3 Ultra‑Heavy Plate (150–300 mm)
Forging/Heavy Rolling → Solution + Quench → Compression Stress Relief (T652) / Stretch Relief (T651) → Aging → Straightening → UT
- Key Notes
- Thickness effect: Strength decreases with thickness due to reduced core quench rate.
- Stress relief: T351/T651/T851/T652 minimize machining distortion for precision parts.
- Aerospace quality: Specify AMS 4037 (Fe ≤0.30%) for improved fatigue life.
- Corrosion: Unclad 2024 requires anodization or coating for outdoor use.


Leave a Reply